Fine Grain Structural steel tube
| NO. | GRADE | SIZE RANGE | STANDARD | ||
| OD/mm | WT/mm | L/m | |||
| 1 | S275J0H | 48~114 | 4~16 | 6~12.2 | EN10210-1 |
| 2 | S275J2H | 114~340 | 4.5~36 | 6~15 | |
| 3 | S355J0H | ||||
| 4 | S355J2H | ||||
| 5 | S355J2H | ||||
| Grade : | S275J0H | ||
| Number: | 1.0149 | ||
| Classification: | Non-alloy structural steel | ||
| Standard: |
|
| Method of deoxidation FN = rimming steels not permitted C < 0.2 for thickness =< 40 mm, CEV < 0.41 / 0.48 for thickness 16 / 65 mm |
| C | Mn | P | S | N |
| max 0.22 | max 1.5 | max 0.035 | max 0.035 | max 0.009 |
| Nominal thickness (mm): | to 3 | 3 - 100 | 100 - 120 |
| Rm - Tensile strength (MPa) | 430-580 | 410-560 | 400-540 |
| Nominal thickness (mm): | to 16 | 16 - 40 | 40 - 63 | 63 - 80 | 80 - 100 | 100 - 120 |
| ReH - Minimum yield strength (MPa) | 275 | 265 | 255 | 245 | 235 | 225 |
| KV - Impact energy (J) | 0° 27 |
| Nominal thickness (mm): | to 40 | 40 - 63 | 63 - 100 | 100 - 120 |
| A - Min. elongation at fracture (%) longitud., | 23 | 22 | 21 | 19 |